正在加载图片...
LAYERED COMPOSITES Vol. 38. No. 1 Slurry of Al, O, Slumy ol A2O3+15wo%mz。2 Slurry of Al,o,+15 vol. "%t-zro, Slip Casting of Paris moid to build up the layered Drying at room temperature for Presintering at 1.C/1 Machining to reach flatness Firing at 1700C/2h under load(P=3 MPa) nder 5x 10 torr vacuum ructural analysis Figure 1. Processing flow chart describing the procedure for making monolithic and laminated composites 2 02004006008001000120014001600 Figure 2. Wall thickness versus time for slip cast alumina slurry